Stainless Steel Materials & Performance

What Do the Markings on Stainless Steel Screw Heads Mean?

For products covered by the applicable standard, A2-70 and A4-80 combine a stainless material designation with a mechanical property class. A manufacturer’s mark provides another identification clue. The short guide below separates these meanings; the product type and marking rules determine how they apply.

In this article
  1. Decode A2-70 within the applicable system
  2. Identify the product and its marking system first
  3. Does A4 prove that the exact alloy is 316L?
  4. What information cannot be encoded in a short head mark?
  5. How should small or unfamiliar markings be investigated?
  6. How can markings support receiving inspection?
  7. Example: two marked lots are mixed in one bin
  8. Common questions
  9. Reference standards

Read the material designation and property class separately, then check the applicable product and marking rules.

Decode A2-70 within the applicable system

Swipe the table sideways to compare every column. Keyboard: use the left and right arrow keys.

Quick guide to stainless screw head markings
Marking componentMeaning and limitation
A2An austenitic stainless material group commonly associated with 304-type materials; it does not identify one exact alloy. The letter A identifies the austenitic family, and the following number distinguishes the material group within this system.
70For a fully loadable product to which the relevant requirements apply, property class 70 corresponds to a minimum tensile strength of 700 N/mm², equivalent to 700 MPa. It is not an installation torque, a design allowable, a safe working stress or a corrosion-life rating.
A4An austenitic stainless material group commonly associated with 316-type materials; A4 alone does not prove that the exact alloy is 316L.
Manufacturer’s markAn identification clue, not a batch test result. Use the receiving record to connect the mark with lot documentation.

First confirm that the product is covered by the relevant marking system. The product type, size and geometry determine which marking requirements apply.

Identify the product and its marking system first

The applicable rules provide the context for decoding a head mark. Product type, size, geometry and the governing standard affect marking requirements. ISO 3506-1 addresses the relevant bolts, screws and studs; tapping screws have a separate framework in ISO 3506-4. A metric machine-screw tensile-class interpretation therefore does not automatically apply to wood or self-drilling screws. The actual product standard establishes the relevant marking and documentation requirements. 1 2

Special head or shank geometries can also limit loadability. The 2020 revision of ISO 3506-1 addresses reduced-loadability products and includes an austenitic class 100. Older summaries that stop at class 80 are therefore incomplete; an unfamiliar number still needs verification against the applicable product and standard. 3

The ASTM Stainless Fastener Standards: 304, 305, 316 & 410 Screws Guide gives broader product-family context before interpreting a mark. Its grade overview does not replace the marking requirements of the applicable product standard.

An example A2–70 head mark connects to product-system, lot-document and unresolved-requirement records in a conceptual traceability map.
Connect the head mark to its system and lotAn example A2–70 head mark connects to product-system, lot-document and unresolved-requirement records in a conceptual traceability map. Conceptual illustration; not to scale and not a measured product result.Open the full-size diagramOpen the full-size diagram.

Does A4 prove that the exact alloy is 316L?

An order specifying a low-carbon grade such as 316L needs material documentation linked to the relevant chemistry requirement. An A4 head stamp cannot supply missing evidence for the exact grade on a drawing.

What information cannot be encoded in a short head mark?

A head mark cannot encode every drawing requirement. Surface cleanliness, passivation, dimensional tolerances, fatigue behavior and a particular corrosion exposure may need separate evidence. A correctly marked screw can still have the wrong length or an unapproved finish.

A conceptual inspection board connects part identification, recording an example head mark, matching lot documents and verifying remaining requirements.
Resolve what the head mark does not tell youA conceptual inspection board connects part identification, recording an example head mark, matching lot documents and verifying remaining requirements. Conceptual planning aid; not a test result or a mandatory manufacturing procedure.Open the full-size diagramOpen the full-size diagram.

How should small or unfamiliar markings be investigated?

Swipe the table sideways to compare every column. Keyboard: use the left and right arrow keys.

Investigating a difficult-to-read head mark
Reading stepUseful evidence
Viewing conditionsThe documentary limits are separate from the practical problem of reading a mark accurately. Consistent lighting and suitable magnification help clarify a doubtful character.
Compare identified piecesCurvature, coating and forming variation can affect legibility, so comparison of several pieces from the same identified package is useful.
Preserve package contextPhotographs linked to the original package label preserve that context.
Resolve uncertain meaningWhen meaning remains unclear, the manufacturer’s marking explanation and product reference provide a more reliable basis than resemblance to an online photograph.

The absence of a readable mark has meaning only in relation to the requirement for that product and size. An unmarked small tapping screw and a machine screw missing a required mark are different inspection cases. A magnet test resolves neither case: magnetic response does not decode a manufacturer identifier or demonstrate compliance with a stated mechanical class.

How can markings support receiving inspection?

Photograph the complete mark beside its package identification. Compare the order, observed characters and lot documents before combining stock.

Where required, link exact-alloy documentation, original wire-heat identity and later surface-treatment records to the delivery lot. A2/A4 and the property-class number do not supply those records or replace inspection of the complete specified product.

Swipe the table sideways to compare every column. Keyboard: use the left and right arrow keys.

Head-marking receiving record
ComparisonEntry or unresolved item
Ordered identification[Product type; size; material designation; property class; applicable standard/contract marking requirement]. Compare these with the package description.
Observed identification[Manufacturer symbol; all visible grade/class characters; legibility; photo reference]. Record what is actually visible.
Package-to-document link[Package/lot ID; inspection-document reference; covered quantity]. Confirm which records apply to the received parts.
Discrepancies[Mixed markings; conflicting fields; damaged or missing identification]. Keep the identity issue unresolved until a documented correction or investigation supports disposition.
Separate performance evidence[Agreed tests/documents; result reference; acceptance decision]. A matching stamp does not replace required verification.

Receiving checks depend on a continuing connection between the package, records and parts. A manufacturer mark usually identifies an organization rather than one individual screw. Two parts bearing the same mark may come from different heats or production lots, which is why the packaging-to-document link remains necessary after unpacking.

The checks described on Quality & Testing for Stainless Steel Screws can be discussed alongside this receiving record.

Example: two marked lots are mixed in one bin

In a hypothetical example, two deliveries contain the same A4-80 machine screw. Their head marks look identical, but their packaging refers to different lots and inspection documents. Once both are poured into an unlabeled bin, the visible mark no longer identifies which document covers an individual piece. Restoration of the original lot allocation from appearance alone may be impossible.

Lot identity preserved through repacking and production issue prevents this loss of traceability. Once mixing has occurred, the affected quantity and agreed disposition process provide the basis for a controlled decision; one conveniently available certificate cannot represent the entire bin without justification. A head mark is most useful when the surrounding traceability system preserves the information that the mark cannot contain.

Common questions

Does an unmarked screw automatically fail inspection?

No. Acceptance depends on whether the applicable product, size and contract require a mark. A missing required mark is a conformity issue. Where marking is not required, suitable packaging and documentation still need to establish identity.

Can the same head marking appear on different production lots?

Yes. Use the receiving record to keep the lot identity and corresponding documents connected.

Should a head mark be accepted when the certificate disagrees?

The disagreement is an unresolved identity question. The affected package, documents and a record of the conflicting fields provide the basis for a traceable correction or investigation. Choosing whichever description best matches the order would leave the cause unresolved. Labeling, documentation and product errors require different dispositions. Once the issue is resolved, evidence linking the accepted parts to the corrected record prevents the same ambiguity from reaching production.

Reference Standards

  1. ISO 3506-1:2020 — Mechanical properties of stainless steel bolts, screws and studs
  2. ISO 3506-4:2025 — Tapping screws with specified grades and hardness classes
  3. SIST official preview — EN ISO 3506-1:2020

These references describe standards and test methods within their stated scope. Listing a standard does not mean that a StainGrip product is certified to it or that a specific batch has passed a test.

Start a conversation

Discuss Your Screw Requirements

Type every visible character and manufacturer symbol, and identify the screw type, dimensions and package/lot reference. State the ordered material/class and the specific marking or document discrepancy you need resolved.

Our technical engineers will contact you within one business day.

Request a Quote →
SEARCH

Search Products & Technical Resources

Enter a product name or technical topic to search.

StainGrip